Liquid epoxy resin for flooring is normally a general purpose bisphenol A grade such as YLE-128, at EEW 184-190 g/eq and 11,000-15,000 mPa·s at 25 °C. It is the cheapest route to epoxy equivalents in Pakistan and India when the hardener is weighed. Cost per equivalent, dilution, and failures follow.

Figure 1. YLE-128 at drum temperature, before it is cut with diluent and filled for a self-levelling pour.
Flooring is where bisphenol A epoxy is bought by the tonne rather than the drum. A buyer in Lahore or Ahmedabad compares three numbers first: price per kilogram, hardener demand, and how much diluent the viscosity forces into the mix.
YLE-128 sits in the middle of that argument. It is the general purpose liquid grade of the bisphenol A family, and the only bisphenol A liquid here listed for flooring. This report prices that discount in epoxy equivalents. No price is published, so every dollar figure below is illustrative.
YLE-128 is the unbranded workhorse of the liquid bisphenol A epoxy resin range. The product page publishes no CAS number for it, so the field is recorded as not published rather than borrowed from a sister grade.
Table 1. Published specification of YLE-128.
Item |
Information |
Grade |
YLE-128 |
Chemical name |
bisphenol A diglycidyl ether |
CAS No. |
not published on the product page |
EEW |
184-190 g/eq |
Viscosity at 25 °C |
11,000-15,000 mPa·s |
Hydrolyzable chlorine |
500 ppm maximum |
Colour |
50 APHA, 2026 catalogue |
Listed applications |
composites, adhesives, coating, flooring |
Packaging, shelf life |
drum; 12 months in the original pack |
EEW is reported as determined by ASTM D1652 titration, with ISO 3001 as the equivalent route. Viscosity is measured at 25 °C according to ASTM D445, and colour per ASTM D1544.
Two quantities are calculated rather than measured: epoxy equivalents per tonne and cost per equivalent. The catalogue prints EEW 184-194 g/eq, the product page 184-190; this report uses the page value and treats the spread in 7.1.
One tonne of YLE-128 at EEW 187 carries 5.35 epoxy equivalents; YLE-127 at EEW 180 carries 5.56. That 3.7% gap is the entire cost argument.
Hardener is dosed against equivalents, so hardener mass per tonne rises as EEW falls: 61.1 kg of YLH-3101 per 100 kg of YLE-127 against 58.8 kg for YLE-128. Hardener cost per equivalent does not move.
Cost per equivalent reduces to (EEW × resin price + AHEW × hardener price) ÷ 1000. YLE-127 wins only while it costs under 96.2% of the YLE-128 price. That ratio decides most purchases of liquid epoxy resin for flooring, and 127 rarely clears it.
The low-chlorine tier is the trap. YLE-128K to 128P carry EEW 165-175 at 3,500-5,500 mPa·s, which reads like cheaper epoxy. They are crystalline electronic potting grades, total chlorine 1,000 down to 300 ppm.
Viscosity is the second bill. At 11,000-15,000 mPa·s, YLE-128 will not level over 3 mm alone; YLE-127 at 8,000-11,000 takes about a third less diluent to reach 6,000 mPa·s.
Table 2. YLE-128 against the three grades a flooring buyer most often weighs instead of it.
Attribute |
YLE-128 |
YLE-127 |
YLE-170 |
YLE-128R |
EEW, g/eq |
184-190 |
176-184 |
160-180 |
185-220 |
Viscosity, mPa·s |
11,000-15,000 |
8,000-11,000 |
2,000-5,000 |
11,000-25,000 |
Hydrolyzable Cl |
500 ppm max |
500 ppm max |
500 ppm max |
printed 2%, unverified |
Equivalents per tonne |
5.35 |
5.56 |
5.88 |
4.55-5.41 |
YLH-3101 demand |
58.8 phr |
59.8-62.5 phr |
64.7 phr |
50.0-59.5 phr |
Crystallisation |
not marked |
not marked |
not marked |
non-crystal type |
Flooring listed |
yes |
no |
no |
yes |
Bisphenol F is the paper alternative: YLE-170 pours at 2,000-5,000 mPa·s with no diluent, but must land below 84-98% of the YLE-128 price to break even, and is not listed for flooring. YLE-128R runs the other way: non-crystal, listed for flooring, EEW to 220.
Hardener demand follows phr = 100 × AHEW ÷ EEW. YLH-3101 publishes AHEW 110 g/eq at 55-60 phr, which back-calculates to a resin EEW of 183-200 g/eq, a band YLE-128 sits inside.
Table 3. Blends of YLE-128 with the AGE reactive diluent and with bisphenol F, calculated at EEW 187 for the base resin.
Blend |
Blend EEW |
Viscosity, mPa·s |
YLH-3101, phr |
Note |
YLE-128, neat |
187 |
13,000 |
58.8 |
will not level at 3 mm |
plus 10 phr YLD-9005 |
183-193 |
6,200 |
56.9-60.1 |
pourable, small cap loss |
plus 15 phr YLD-9005 |
182-196 |
4,500 |
56.1-60.4 |
usual cost-line compromise |
plus 20 phr YLD-9005 |
180-199 |
3,400 |
55.3-61.1 |
recheck solvent resistance |
70:30 with YLE-170 |
182 |
8,800 |
60.4 |
no monofunctional cap |
Two cautions apply. Those viscosities are logarithmic mixing estimates from mid-band values, not measurements, and the EEW bands widen because the diluent is published as 155-285 g/eq. YLD-9005 also carries one epoxy group per molecule, so it caps a chain.
Filler dominates mass, binder dominates cost. A 3:1 screed on 100 kg of YLE-128 holds 58.8 kg of hardener and 476 kg of filler, so binder is 25% of the mass. At assumed prices of USD 2.30, 3.20 and 0.09 per kg, illustrative only, it is 91% of the cost.
That ratio decides where to negotiate. A 5% resin rise adds about USD 11.5 per tonne of floor; a 5% filler rise adds 2.1.
The operating window is set by the hardener. YLH-3101 gels in 40-70 min at 25 °C, surface dries in 3.5 h, hard dries in 7 h, and at 5 °C those stretch to 10 h and 24 h.
The YLH-3101 hardener is listed for self-levelling floor topcoats, the reference here. Five points carry most of the risk:

Figure 2. Self-levelling compound at 3 mm, spread in batches that match a 40-70 min gel time.
Four floor types carry almost all the volume in cost-sensitive markets, and each one fails for a different reason.
The volume application is a 1-3 mm coloured wear layer. Dosage runs 100:58.8 with 1.2-1.5 kg of binder per m² plus 3:1 filler. A surface that scratches white after a month almost always carries more than 15 phr of diluent.
Binder content of 25-30% by mortar mass gives the acid and spill resistance a dairy or plating shop needs. Below 25% the mortar turns porous, above 35% it cracks in shrinkage. Quartz grading follows binder content, not the reverse.
A 3-4 mm joint-free lining over bund walls takes the same 100:58.8 binder, sometimes accelerated with 1,3-BDX for early rain resistance. Still air in a sump is the hazard: amine carbonate skins over and the next coat will not bond.
At 0.3-0.4 kg/m² the same resin binds dust and keys the screed to the slab. On a slab poured three weeks earlier, moisture drives through and blisters the film. 1,3-BDX is the grade to test there, since wet-surface adhesion is claimed for it and not for bisphenol A.
Table 4. Floor types, dose windows and the failure each one is prone to.
Application |
Dose |
Function |
Failure point |
Self-levelling topcoat |
1.2-1.5 kg/m² binder |
flow, gloss, wear |
white scratch above 15 phr diluent |
Chemical-resistant screed |
25-30% binder by mass |
acid and spill resistance |
porosity below 25%, cracks above 35% |
Containment lining |
3-4 mm, two coats |
barrier without joints |
amine carbonate in still air |
Primer on damp slab |
0.3-0.4 kg/m² |
adhesion, dust binding |
blistering on a cold slab |
Car park deck |
2-3 mm, sand broadcast |
abrasion, tyre marking |
yellowing under skylights |

Figure 3. A 2 mm deck coating on YLE-128; the aromatic backbone limits it to interiors or to a pigmented topcoat.
Four jobs should not be quoted on grade 128. UV topcoats yellow on the aromatic backbone; hot solvent immersion needs a bisphenol F epoxy resin; castings over 50 mm run away on exotherm. A spec capping total chlorine near 300 ppm is an electronic job.
The EEW spread matters more than buyers expect. A lot titrating at 194 g/eq against a recipe set at 58.8 phr lands 3.7% amine-rich, which plasticises the film. Retitrate before changing anything else.
Three tests catch most bad lots: EEW by titration, water by Karl Fischer, colour against a Gardner or APHA standard. Run each on a duplicate sample and hold the drum on a 5 g deviation.
The product page states drum packaging and at least 12 months from manufacture in the original pack. A general purpose grade can crystallise in a cold warehouse; warm to 50-60 °C, roll the drum, and confirm the crystals are gone.
Safety data sits with the MSDS, not this report. Uncured resin is a skin sensitiser and amine hardeners are corrosive as supplied. The TDS, MSDS and COA for the delivered lot override every number here.
It depends on two numbers. YLE-127 stays cheaper per epoxy equivalent only while it costs under 96.2% of the YLE-128 price. If the plant also buys 15 phr of diluent, the 3.8% gap usually closes.
At EEW 187, one tonne of YLE-128 takes 588 kg of YLH-3101, which is the 58.8 phr figure. At 190 g/eq demand falls to 579 kg; at 184 g/eq it rises to 598 kg.
No. Neat YLE-128 at 11,000-15,000 mPa·s will not level to 1 mm over a large area, and solvent thinning leaves pinholes. Use 10-15 phr of a reactive diluent, or start from YLE-127 at 8,000-11,000 mPa·s.
Amine carbonate. Moisture and carbon dioxide react with unreacted amine at the film surface when the slab sits at or below dew point. The fix is schedule: prime later in the day, keep the slab 3 °C above dew point, and never coat a slab that is still cooling.
Above roughly 15 phr of a monofunctional diluent, crosslink density drops enough to show in solvent rubs. Verify with a 24 h immersion coupon in the actual spill medium rather than trusting a generic table.
EEW, hydrolyzable chlorine, water and colour, each against the lot number. Reject or retitrate any lot above 190 g/eq if the recipe was written at 58.8 phr, because the hardener dose is no longer stoichiometric.
YLE-128 is a cost instrument, not a performance grade. It delivers 5.35 epoxy equivalents per tonne at 11,000-15,000 mPa·s, and stays the cheaper epoxy only while it holds 3.8% below the YLE-127 price.
Hardener and diluent decide whether that saving survives. Binder is a quarter of a filled screed by mass and about 91% of its cost at the illustrative prices used here, so negotiation belongs on the resin line, not the filler pile.
1. Yolatech product page: https://www.yolatech.com/bisphenol-a-epoxy-resin (accessed 2026-11-20).
2. Yolatech product page: https://www.yolatech.com/curing-agent-ylh-3101 (accessed 2026-11-20).
3. Yolatech product page: https://www.yolatech.com/allyl-glycidyl-ether-yld-9005 (accessed 2026-11-20).
4. Yolatech Technical Data Sheet (TDS) for YLE-128, EEW 184-190 g/eq (available on request).
5. ASTM D1652, epoxy content of epoxy resins (EEW).
6. ASTM D445, kinematic viscosity.
7. ASTM D1544, Gardner color of transparent liquids.