Language :
Benzyl glycidyl ether YLD-6021 is a monofunctional aromatic diluent at 208-228 g/eq and 2-8 mPa·s, picked for potting when colour and chloride allow. At 20 phr it lifts blend EEW so amine demand falls, not rises; the same load brings 750 ppm hydrolyzable chloride, and that number settles the choice.

Figure 1. YLD-6021 is a water-clear liquid; the published colour ceiling is APHA 50.
Viscosity limits most room-temperature epoxy work. A liquid bisphenol A resin such as YLE-128 runs at 11,000-15,000 mPa·s, too thick for potting fine windings or a brush coat without solvent. A reactive diluent lowers that figure and stays in the film.
Several diluents in this catalogue bring that figure down, and choosing between them on viscosity alone is a mistake: functionality, colour ceiling and chloride load move with the choice. This report sets benzyl glycidyl ether YLD-6021 (CAS 89616-40-0) against three of them and states the arithmetic behind each decision.
The CAS number sits in the product page intro line, not the specification table.
Table 1. Identity of benzyl glycidyl ether YLD-6021.
Item |
Information |
Chemical name |
Benzyl glycidyl ether |
CAS No. |
89616-40-0 |
Molecular formula |
C10H12O2 (calculated) |
Molecular weight |
164.20 g/mol (calculated) |
Theoretical EEW |
164.2 g/eq, one oxirane per molecule (calculated) |
Appearance |
Transparent liquid |
Package |
Drum |
Seven parameters are published, with no cure data and no thermal properties.
Table 2. Published specification of YLD-6021 with the method applied to each parameter.
Parameter |
Published value |
Method |
Colour, APHA |
Max. 50 |
APHA scale |
Viscosity at 25 °C, mPa·s |
2-8 |
ASTM D445 |
EEW, g/eq |
208-228 |
ASTM D1652, ISO 3001 |
Hydrolyzable chloride, % |
Max. 0.2 |
Titration |
Inorganic chlorine, ppm |
Max. 50 |
Titration |
Water, % |
Max. 0.1 |
ASTM E203 |
Epoxy equivalent weight is determined by titration according to ASTM D1652 or ISO 3001, water content according to ASTM E203. Viscosity is quoted at 25 °C; the page names no method, and ASTM D445 is the standard used across this catalogue. With no standard deviation or replicate count published, these figures are limits, not typicals.
The published EEW of 208-228 g/eq sits well above the 164.2 g/eq calculated for the pure monomer, and that gap decides the arithmetic. A grade at 218 g/eq carries about three quarters of the epoxy content of the pure monomer; the rest is non-reactive. Substituting 164 overstates epoxy equivalents by a third, and the hardener weight follows.
Benzyl glycidyl ether carries one oxirane ring on a short ether chain capped by a benzene ring, and no hydroxyl. That absence is why viscosity lands at 2-8 mPa·s. Bisphenol A resin is thick because its backbone hydroxyls hydrogen-bond; a benzyl ether has nothing to bond with.
At 15 phr it takes a 13,000 mPa·s resin to about 4,660 mPa·s, the working range for casting small housings (Table 5).
Reactivity is where the monofunctionality costs. Each molecule reacts once and stops, capping a chain end rather than extending the network, so crosslink density falls with the monofunctional fraction. The aromatic ring recovers part of that, and the page claims a high heat deflection temperature without publishing an HDT value to size it.
Table 3 lines YLD-6021 up against three grades; all colour values are APHA, not Gardner.
Table 3. Selection matrix: benzyl glycidyl ether YLD-6021 against three diluents, values as published on each product page.
Property |
YLD-6021 |
YLD-6001 |
YLD-9004A |
Chemical type |
Benzyl glycidyl ether |
Glycidyl phenyl ether |
Butyl glycidyl ether |
Functionality |
1 |
1 |
1 |
EEW, g/eq |
208-228 |
Not published |
147-157 |
Viscosity at 25 °C, mPa·s |
2-8 |
2-8 |
Max. 2 |
Colour, APHA |
Max. 50 |
Max. 50 |
Max. 20 |
Hydrolyzable chloride |
Max. 0.2 % |
Not published |
Max. 0.1 % |
Effect on blend EEW |
Raises |
Raises |
Lowers |
The last two rows drive the pick. Difunctional 1,6-hexanediol diglycidyl ether YLD-6008 at 142-155 g/eq pulls blend EEW down and hardener demand up; YLD-6021 at 218 g/eq does the opposite. At 20 phr the two recipes need 12.9 phr against 11.5 phr, a gap no batch sheet shows.
Odour and colour settle the rest. Butyl glycidyl ether YLD-9004A reaches max. 2 mPa·s at APHA 20, both better than YLD-6021, and pays with a sharper smell on an open line.
Table 4 orders them by cost of getting them wrong.
Table 4. Diluent decision sequence for a room-temperature bisphenol A system: condition, action, governing limit.
Application condition |
Action |
Governing limit |
Ionic limit under 500 ppm |
Stop; settle the COA first |
2,000 ppm hydrolyzable Cl |
Light or white topcoat |
Move to YLD-9004A |
APHA 50 vs APHA 20 |
Crosslink density first |
Use difunctional YLD-6008 |
Monofunctional capping |
Open pot, operators close |
Keep YLD-6021, skip the butyl |
Odour claim: neat liquid |
Target 3,000-5,000 mPa·s |
Set 15-20 phr |
Log mixing rule, coupon check |
Structural part over 20 phr |
Reduce loading or accept lower HDT |
A quarter of binder capped |
Once the grade is fixed, hardener demand follows the epoxy equivalents in the blend, not the resin mass alone.
EEW(blend) = (100 + L) ÷ (100 ÷ EEW(resin) + L ÷ EEW(diluent)), with L as diluent loading in phr
phr(amine) = 100 × AHEW ÷ EEW(blend)
Table 5 applies both to liquid bisphenol A epoxy resin YLE-128 (EEW 184-190 g/eq, 11,000-15,000 mPa·s) with YLD-6021 at 0-30 phr. Viscosity comes from the logarithmic mixing rule, an approximation to check on a coupon before scaling.
Table 5. Blend properties of YLD-6021 in YLE-128; viscosity estimated, hardener calculated at AHEW 20.6 g/eq.
YLD-6021, phr |
Blend EEW, g/eq |
Viscosity, mPa·s |
DETA, phr blend |
DETA, phr resin |
0 |
187.0 |
13,000 |
11.0 |
11.0 |
5 |
188.3 |
8,940 |
10.9 |
11.5 |
10 |
189.4 |
6,360 |
10.9 |
12.0 |
15 |
190.5 |
4,660 |
10.8 |
12.4 |
20 |
191.5 |
3,510 |
10.8 |
12.9 |
30 |
193.3 |
2,120 |
10.7 |
13.9 |
A 120 kg batch of 100 kg YLE-128 plus 20 kg YLD-6021 lands at 191.5 g/eq and takes 12.9 kg of diethylenetriamine at AHEW 20.6 g/eq, or 10.75 phr on blend mass. Both describe one recipe; quoting one without its basis is the usual dosing error at scale.
Chloride scales with loading. At 20 phr the diluent brings about 40 g of hydrolyzable chloride into that batch against 50 g from the resin, near 750 ppm; at 30 phr, 846 ppm. With an ionic limit under 500 ppm neither loading passes, and the COA value has to be settled first.
Twenty phr is a sensible ceiling for structural work. At 30 phr viscosity falls to 2,120 mPa·s, but a quarter of the binder is monofunctional and heat distortion shows it.
YLD-6021 disperses without high shear, which changes the sequence, not the equipment.

Figure 2. Diluent is metered into the resin by mass; low-shear mixing is enough at 2-8 mPa·s.
A 20 phr blend holds less resin per unit volume, so a thick casting runs cooler while a thin film skins sooner. Re-check the cure schedule when loading changes.
Three uses appear on the page, each loading following from Table 4.
Table 6. Applications of YLD-6021, with the loading it supports and the governing limit.
Application |
Role in the process |
Loading, phr |
Governing limit |
Electronic potting |
Cavity fill and wetting of windings |
10-20 |
Hydrolyzable chloride budget |
Coating |
Solvent-free let-down for brush or roller |
15-25 |
Colour ceiling at APHA 50 |
Construction adhesive |
Penetration into rough substrate |
10-15 |
Chain termination at high load |

Figure 3. Potting a wound assembly: 10-20 phr of YLD-6021 brings a bisphenol A system into the 3,500-6,400 mPa·s range.
Potting is the demanding case. A 20 phr blend at 3,510 mPa·s wets a winding in one pass, but it carries 750 ppm hydrolyzable chloride, and that number, not viscosity, decides insulation tests on high-impedance circuits.
Four limits rule uses out, each a selection filter.
The 4-tert-butylphenyl glycidyl ether YLD-6004 page repeats the 2-methylphenyl description word for word, so verify that grade from its table alone.
Incoming check covers viscosity at 25 °C, colour, water and EEW on the COA sample. Viscosity and EEW catch most off-spec lots; a wet batch shifts in viscosity before the water figure moves.
Drums keep 12 months in original packing at ambient temperature, away from flame and sunlight.
Safety data sits in the Material Safety Data Sheet; treat the liquid as a skin sensitiser until the MSDS says otherwise. No RoHS or REACH status is claimed here; that comes from the supplier's declaration.
Choose it when the ionic limit sits above 500 ppm, the topcoat is not colour-critical and Tg can give up a little: it is the only grade here that cuts viscosity while lowering amine demand. Move to YLD-9004A for APHA 20, or YLD-6008 when crosslink density beats flow.
Ten to twenty phr covers most work. At 20 phr a 13,000 mPa·s resin drops to 3,500 mPa·s; 30 phr reaches 2,120 mPa·s but makes a quarter of the binder monofunctional.
No. YLD-6021 is benzyl glycidyl ether, CAS 89616-40-0, at EEW 208-228 g/eq; YLD-9004A is butyl glycidyl ether, CAS 2426-08-6, at 147-157 g/eq. Both are monofunctional, but blend EEW moves opposite ways.
Yes. Capping chain ends drops crosslink density and Tg together. How far depends on the hardener, since the page lists no Tg or HDT; the aromatic ring offsets part of it, and a coupon settles the rest.
The specification allows max. 0.2 % hydrolyzable chloride, or 2,000 ppm. At 20 phr in a resin carrying 500 ppm the blend lands near 750 ppm; at 30 phr, 846 ppm.
It can, and it stays in the film, so there is no flash-off step and no diluent VOC. Two constraints apply: hardness drops at high loading, and APHA 50 bars light topcoats that the butyl grade would pass.
Benzyl glycidyl ether YLD-6021 cuts viscosity to 2-8 mPa·s while moving blend EEW up, so amine demand falls as loading rises — the reverse of difunctional grades. At 20 phr in YLE-128 the blend reaches 191.5 g/eq and 3,500 mPa·s, needing 12.9 kg of diethylenetriamine per 100 kg of resin.
Selection then turns on two limits, not viscosity. Chloride at 2,000 ppm puts the blend at 750 ppm at 20 phr, ruling out high-impedance potting unless the COA comes lower; chain termination rules out structural parts above 20 phr.
1. Yolatech product page: https://www.yolatech.com/benzyl-glycidyl-ether-yld-6021 (accessed 2026-11-16).
2. Yolatech Technical Data Sheet (TDS) for YLD-6021, benzyl glycidyl ether, CAS 89616-40-0, on request.
3. Yolatech Certificate of Analysis (COA) for YLD-6021, batch values, on request.
4. ASTM D1652, epoxy content of epoxy resins (EEW).
5. ISO 3001, determination of epoxy equivalent.
6. ASTM D445, kinematic viscosity.
7. ASTM E203, water content by Karl Fischer titration.