Cycloaliphatic amine curing agent YLH-3618 is a modified cycloaliphatic amine at 300-500 mPa·s, 260-290 mg KOH/g amine value and AHEW 112 g/eq. At 60 phr it enters the Ancamine 1618 recipe unchanged, but AHEW, gel time and colour do not follow. The recipe matches; the window itself only partly does.

Figure 1. YLH-3618 as supplied: a pale, 300-500 mPa·s modified cycloaliphatic amine.
A 60 phr dosage at EEW 190 is the first number buyers compare, and on it YLH-3618 and Ancamine 1618 are identical. Both are modified cycloaliphatic amines for solvent-free flooring and tank linings, where low viscosity and pale colour decide the formulation.
This report compares published figures only. YLH-3618 values come from the 2026 Yolatech curing agent catalogue, page 9; Ancamine 1618 values from the supplier's technical data sheet. Dosages are recalculated from AHEW and EEW, and each derived number carries its arithmetic.
YLH-3618 carries an AHEW of 112 g/eq and a recommended 60 phr at EEW 190, the two figures needed to build a recipe. The grade has no standalone product page, so the catalogue entry is the authoritative public source.
Table 1. Published identification and specification of YLH-3618 (Catalogue 2026, page 9).
Item |
Published value |
Grade |
YLH-3618 |
Chemical type |
Modified cycloaliphatic amine |
Colour, Gardner |
3 max |
Viscosity at 25 °C |
300-500 mPa·s |
Amine value |
260-290 mg KOH/g |
Amine hydrogen equivalent weight |
112 g/eq |
Recommended dosage, EEW 190 |
60 phr |
Pot life |
40 min |
Thin film set time |
7 h |
CAS number |
Not published |
Density, flash point |
Not published |
Pack size, shelf life |
Not published |
Three kinds of figure appear here, with different weight. Catalogue values are supplier typicals, and no test method is named, so the list below is the conventional route for this class.
Colour is read according to ASTM D1544, viscosity according to ASTM D445, amine value according to ISO 9702, water content according to ASTM E203; resin EEW by ASTM D1652 or ISO 3001. Derived dosages are calculated, not measured.
Ancamine 1618 figures come from the supplier data sheet (EMEA edition): 450 mPa·s, amine value 260-285 mg KOH/g, AHEW 115 g/eq, 60 phr at EEW 190, gel time 50 min on 150 g at 25 °C. Naming the source lets a reader check the comparison.
An AHEW of 112 g/eq means 112 g of YLH-3618 carries one mole of active hydrogen, so 60 phr supplies 0.536 eq against 0.526 eq of epoxy in 100 g of EEW 190 bisphenol-A resin. The two sit within 1.8%, which is why the dosage rounds to 60.
The amine value does not agree with that reading. Dividing 56,100 by the 275 mg KOH/g midpoint gives 204 g/eq, 82% above the published 112. Ancamine 1618 behaves the same way: 56,100 ÷ 272 = 206 g/eq against a stated 115.
Both suppliers calibrate AHEW so the recommended phr lands on stoichiometry, while amine value counts all titratable nitrogen, modifier included. Use AHEW for the recipe, amine value for inspection; converting one into the other doubles the dosage.
Five of the nine published properties match, and the differences left are one Gardner step and one missing cold-cure datum. Table 2 sets them side by side.
Table 2. YLH-3618 against Ancamine 1618 on published figures.
Property |
YLH-3618 |
Ancamine 1618 |
Difference |
Chemical type |
Modified cycloaliphatic amine |
Modified cycloaliphatic amine adduct |
Same class |
Colour, Gardner |
3 max |
Below 2 |
One step deeper |
Viscosity at 25 °C |
300-500 mPa·s |
450 mPa·s |
Competitor inside range |
Amine value |
260-290 mg KOH/g |
260-285 mg KOH/g |
Overlapping |
AHEW |
112 g/eq |
115 g/eq |
-3 g/eq, -2.6% |
Dosage at EEW 190 |
60 phr |
60 phr |
Identical |
Working life |
40 min pot life, mix mass not stated |
50 min gel time, 150 g at 25 °C |
Not like-for-like |
Thin film set, 25 °C |
7 h |
7 h |
Equal |
Thin film set, 10 °C |
Not published |
19.5 h |
No datum published |
The 40 min and 50 min entries cannot be subtracted. One is a catalogue pot life with no stated mass; the other a gel time on 150 g. In practice the gap must be measured on the mix actually used, because pot life falls as batch mass rises.
Colour decides where the product can go. A reading of 3 max suits a pigmented floor and is marginal under a clear topcoat. If the approved formulation is a water-white sealer, that one Gardner step is a barrier.
The dosage follows one equation, phr = 100 × AHEW ÷ EEW, which at EEW 190 returns 58.9 phr rather than the round 60 printed in the catalogue.
Table 3. Dosage of YLH-3618 against resin EEW, calculated from phr = 100 × 112 ÷ EEW.
Resin EEW, g/eq |
Calculated phr |
Hardener per 100 kg resin |
Mix ratio by weight |
175 |
64.0 |
64.0 kg |
100:64 |
182 |
61.5 |
61.5 kg |
100:62 |
190 |
58.9 |
58.9 kg |
100:59 |
195 |
57.4 |
57.4 kg |
100:57 |
At 60 phr the hardener is 37.5% of the mixed mass, so a 25 kg kit splits into 15.6 kg resin and 9.4 kg hardener. A split error on that 5:3 basis shows in the cured film within a day.
By volume the pair runs about 1.48:1, taking 1.16 g/cm³ for the resin and 1.03 g/cm³ for the hardener. Density is not published for YLH-3618: 1.03 is the competitor figure, for orientation only, so weigh until the COA confirms it. Other grades move the same equation, with YLH-9101 at AHEW 92 g/eq asking about 48 phr.
This cycloaliphatic amine curing agent at 300-500 mPa·s keeps the mixed viscosity low enough for self-levelling, and the 7 h set returns a floor next shift. The window is set by the 40 min pot life.
Three rules cover most of the field experience with this grade:
- Pour within 20 min of mixing. A 20 kg batch held for half its pot life is already thickening.
- Hold air and substrate at 15 °C or above. No low-temperature set time is published, so a 10 °C pour is untested.
- Keep humidity under 75% in the first hours. The catalogue lists yellowing resistance but not blush resistance, and free amine on a damp surface forms a carbamate film.

Figure 2. Self-levelling floor: low mixed viscosity lets a 2-3 mm film flow out.
Four application families are listed for YLH-3618, each leaning on a different property. Flooring depends on viscosity and pot life, linings on chemical resistance and gloss, adhesives on wetting. The YLH-3023 grade covers the thinner end of the same work, with YLH-6004 and YLH-5101 covering other viscosities.
Table 4. Application fit for YLH-3618 with the constraint that governs each use.
Application |
Why it fits |
Constraint |
Self-levelling flooring |
300-500 mPa·s flows to a 2-3 mm film |
40 min pot life caps pour size |
Tank and bund linings |
High gloss, good chemical resistance |
No immersion data published |
Heavy-duty floors |
7 h set returns the area next shift |
Colour 3 rules out pale topcoats |
Adhesives, encapsulation |
Low viscosity wets filler and inserts |
Exotherm in thick sections |

Figure 3. Tank lining in progress: gloss and chemical resistance drive the specification.
Five gaps limit what can be claimed, and none closes by calculation. The catalogue publishes no CAS number, density, flash point, pack size or shelf life, so transport papers and storage limits come from the COA and MSDS of each batch.
A Gardner colour of 3 is not a clear-coat specification. It suits pigmented floors, mortar and grout, and fails where a water-white finish sells the job.
No 10 °C datum is published, while the competitor lists 19.5 h at that temperature. A winter pour is unqualified: test the mix at the intended temperature, or move the work indoors.
Chemical resistance is described as good and nothing more: no media table, concentration or immersion duration. Concentrated acids, chlorinated solvents and hot caustic each need a test.
Five checks cover a delivery, and colour plus amine value catch most off-spec drums. Water content matters because a wet hardener fogs the film and shifts the titrated value.
Table 5. Incoming inspection schedule for YLH-3618.
Check |
Method |
Accept if |
Why it matters |
Colour |
ASTM D1544 |
3 max |
Darker drums show in clear films |
Viscosity |
ASTM D445 at 25 °C |
300-500 mPa·s |
Thick batches hold air |
Amine value |
ISO 9702 |
260-290 mg KOH/g |
Tracks active content |
Water content |
ASTM E203 |
Limit agreed with supplier |
Water fogs the film |
Dosage |
phr from the COA AHEW |
58-61 phr at EEW 190 |
Wrong AHEW moves stoichiometry |
Pack size and shelf life are not published: settle both in the order, then store per the amine class, ventilated, out of sunlight and away from acids.
Modified cycloaliphatic amines are corrosive and skin-sensitising by class, so gloves, eye protection and ventilation belong in the work instruction, with the MSDS governing. No RoHS, REACH or UL 94 statement is published; ask for the declaration per shipment. Where this report and a batch TDS, MSDS or COA disagree, the batch document governs.
For dosage, yes. Hardener mass, mix ratio and the 7 h set carry over. Colour, cold cure and pot life do not, so run a 2 kg trial before releasing a batch.
60 phr is the catalogue figure; 58.9 phr is exact, from 100 × 112 ÷ 190. Anything from 58 to 61 phr cures, and the middle of the band leaves the least free amine.
They come from different tests. The catalogue pot life states no mass or temperature; the competitor 50 min is a gel time on 150 g at 25 °C. Measure both when the batch arrives.
No low-temperature data are published, so a cold pour is unqualified. The competitor lists 19.5 h at 10 °C; without an equivalent figure, heat the space or test at the intended temperature.
The catalogue lists yellowing resistance but not blush resistance, so treat blush as possible. Keep humidity under 75% and sand any soapy film before recoating.
At 60 phr the kit splits 15.6 kg resin to 9.4 kg hardener, a 5:3 ratio by weight. The 1.48:1 volume ratio rests on an assumed density, so weigh both parts.
YLH-3618 matches Ancamine 1618 on the number that starts a formulation, 60 phr at EEW 190. The differences appear later: 112 g/eq against 115, Gardner 3 against below 2, and a 40 min pot life against a 50 min gel time measured differently.
Three checks decide the swap: colour against the approved film, pot life on the real batch mass, and a 28-day immersion test on the actual reagent.
1. Yolatech Curing Agent Catalogue 2026, page 9, product entry for YLH-3618 (technical data sheet, available on request).
2. ASTM D1652, epoxy content of epoxy resins (EEW).
3. ISO 3001, determination of epoxy equivalent.
4. ISO 9702, amine group nitrogen content of amine epoxide hardeners.
5. ASTM D445, kinematic viscosity.
6. ASTM D1544, Gardner color of transparent liquids.
7. ASTM E203, water content by Karl Fischer titration.
8. Yolatech Technical Data Sheet, Material Safety Data Sheet and Certificate of Analysis for YLH-3618 (available on request).