Tetrafunctional epoxy resin YLSE-721 is a four-epoxy-group aniline epoxy sold in three versions with EEW 105-125 g/eq. Chemically it is 4,4'-methylenebis(N,N-diglycidylaniline); its rigid core pushes crosslink density and heat resistance past bisphenol A resins. Grade data, dosage and limits follow.

Yellow tetrafunctional aniline epoxy resin YLSE-721 in a glass beaker on a laboratory bench

Figure 1. YLSE-721 ships as a yellow viscous liquid; the three grades share one appearance specification.

1. Introduction

Filament winding and high-temperature adhesive work both punish difunctional resins. Bisphenol A diglycidyl ether networks soften well before 150 °C, so formulators needing mechanical properties near 200 °C move to multifunctional aniline epoxies. Tetrafunctional epoxy resin YLSE-721 is the Yolatech grade for that job: the product page names filament-wound composites, long pot life at process temperature and high Tg.

This report compiles what the YLSE-721 product page publishes, separates it from calculated values, and works through grade selection, dosage and field limits. Numbers stop where the page stops. Nothing here replaces the current TDS.

2. Materials and Methods: Tetrafunctional Epoxy Resin YLSE-721 Grade Data

2.1 Product Identification and Specification

Table 1 collects identity data. Molecular weight and the theoretical equivalent are calculated from the chemical name; the CAS number comes from third-party databases because the page does not list it.

Table 1. Identity of 4,4'-methylenebis(N,N-diglycidylaniline) YLSE-721.

Item

Information

Chemical name

4,4'-methylenebis(N,N-diglycidylaniline)

CAS No.

Not published on the product page; 28768-32-3 per third-party databases, confirm on the COA

Molecular formula / MW

C25H30N2O4 / 422.52 g/mol, calculated from the chemical name

Functionality

4 epoxy groups (stated on the page: tetrafunctional)

Theoretical EEW

105.6 g/eq, calculated (422.52 / 4); published window 105-120 g/eq for YLSE-721

Table 2 reproduces the published grade table; the versions share one chemistry and differ in viscosity, price and purity positioning.

Table 2. Published specification of the three YLSE-721 grades.

Item

YLSE-721L

YLSE-721C

YLSE-721

Appearance

Yellow liquid

Yellow liquid

Yellow liquid

Color, Gardner

10 or below

10 or below

10 or below

Viscosity, cps (see 7.1)

6000-11000 (25 °C)

3000-7000

3000-7000

EEW, g/eq

110-125

110-125

105-120

Volatiles, %

0.6 or below

0.6 or below

0.6 or below

Positioning

Lower viscosity

Lower price

High purity

2.2 Test Methods and Data Sources

Three data classes are kept apart. Published values come from the product page. Calculated values, such as the 105.6 g/eq theoretical equivalent, follow from arithmetic on published facts. Third-party values, such as CAS 28768-32-3, carry their own attribution and are not treated as supplier data. In release testing the epoxy equivalent is normally determined by titration according to ASTM D1652 or ISO 3001, and Gardner color is measured according to ASTM D1544; the page does not state its internal methods, so the inspection plan in 7.2 fixes them instead.

3. Results and Discussion

3.1 Structure and Reactivity: Four Epoxy Groups on a Rigid Aniline Core

Four epoxy groups per 422.52 g/mol molecule set the ceiling on crosslink density. A fully reacted YLSE-721 network carries roughly twice the junction density of a difunctional resin of similar equivalent weight, the structural reason behind the high Tg and hot mechanical retention.

Two secondary effects matter in practice. Tertiary aniline nitrogens left after glycidylation catalyze their own cure, which supports the long pot life the page describes; the same activity means accelerator dosing must be trimmed, not added blindly. The aromatic backbone resists chain scission, backing the radiation and chemical resistance claims. Pot life is not a free gift: when the winding bath sits warm for hours, viscosity still drifts, and bath turnover discipline decides the day's consistency.

3.2 Comparison with Alternative Systems

Table 3 sets YLSE-721 against the two closest alternatives in the portfolio: trifunctional aminophenol YLSE-0500 and liquid tetrafunctional YLD-1240. All values are published, viscosity at 25 °C where stated.

Table 3. Property comparison of YLSE-721 with alternative multifunctional systems.

Attribute

YLSE-721 (this product)

YLSE-0510 (alternative)

YLD-1240 (alternative)

Functionality

4 (tetrafunctional)

3 (trifunctional)

4 (tetrafunctional)

EEW, g/eq

105-120

93-106

95-110

Viscosity, cps at 25 °C

3000-7000 (721/721C)

400-900

1600-3000

Trade-off

Highest Tg potential, stiff processing

Easiest flow, lower crosslink density

Lowest viscosity among the tetrafunctional grades

Best fit

Filament-wound hot-service vessels

Fast wet-out laminating

Casting where heat resistance meets flow

The hierarchy is strict. If the part must hold stiffness near 200 °C, the tetrafunctional aniline core wins, and the viscosity price is paid through heated lines or a diluent such as YLD-6008 hexanediol diglycidyl ether. If wet-out speed dominates and service temperature stays moderate, the low-viscosity trifunctional N,N-diglycidyl-4-glycidyloxyaniline YLSE-0500 series fits better. The liquid tetrafunctional grade YLD-1240 sits between them, while YLSE-0600 aniline epoxy resincovers cases needing a pendant glycidyl ether for flexibility.

4. Formulation and Dosage Calculation

Dosage follows the standard equivalent relationship: phr = 100 × AHEW ÷ EEW, with AHEW the amine hydrogen equivalent weight of the curative and EEW the epoxy equivalent of the resin. Table 4 evaluates both ends of the published YLSE-721 window, 105 and 120 g/eq, with curatives documented on the Yolatech site. The anhydride row applies the 0.85 empirical factor.

Table 4. Calculated curative demand for YLSE-721 at the published EEW limits.

Curative

AHEW, g/eq

phr at EEW 105

phr at EEW 120

PACM cycloaliphatic diamine

52.6 (calculated)

50.1

43.8

MHHPA liquid anhydride, factor 0.85

168.19 (calculated)

136.1

119.1

YLH-9101 modified amine

92

87.6

76.7

YLH-3002 modified amine

182

173.3

151.7

Dosage matters. Treat every number in Table 4 as a calculated starting point, not a specification. Aerospace practice cures aniline tetrafunctional resins with aromatic amines, outside the current Yolatech portfolio; those systems typically run a staged schedule with a postcure well above 150 °C to reach the promised Tg. When a first trial is mixed, gel time and a DSC scan on the actual curative lot decide the schedule; accelerator level swings gel time by hours. The theoretical equivalent, 105.6 g/eq, sits inside the published window, a useful cross-check that the grade is close to neat monomer.

5. Processing Notes and Operating Window

Handling a 3000-11000 cps aniline resin is mostly heat management and bath hygiene.

- Warm the resin gently before metering; even 40-50 °C cuts batching time sharply.
- Degas after adding curative; entrained air in a filament-wound wall becomes a void path.
- Keep bath temperature steady during winding; pot life still degrades once the batch is catalyzed.
- Dilution with a mono- or difunctional ether lowers viscosity but trades away Tg; weigh that before adding much.
- Postcure above 150 °C where the part geometry allows; undercured aniline networks look done and creep in service.

Filament winding machine winding carbon fiber rovings onto a rotating mandrel

Figure 2. Filament winding, the first process the page names for YLSE-721; bath viscosity stability and degassing decide quality.

6. Applications: Filament Winding and Structural Adhesive

The page names two application fields: carbon and glass fiber composites, and structural adhesive for 200-260 °C service. Table 5 lists each with the resin's role.

Table 5. Published application fields and the role of YLSE-721 in each.

Application

Role of YLSE-721

Process note

Carbon fiber composites

Matrix resin for high-temperature parts

Filament winding or prepreg route

Glass fiber composites

Matrix resin where cost is tighter

721C positioning favors volume

Structural adhesive, 200-260 °C

Heat-resistant adhesive base

Joint design must share the thermal load

Carbon fiber panels bonded with a thin amber epoxy structural adhesive layer

Figure 3. In the 200-260 °C structural adhesive field, the aniline network holds the bondline; bisphenol A systems creep.

7. Limitations and Material Verification

7.1 Known Limitations and Unsuited Uses

Three published facts deserve a caution flag. First, the viscosity row of the grade table carries the header "cps at 50 °C", yet the YLSE-721L cell is annotated "25 °C", and the L grade is labeled "Lower viscosity" while showing 6000-11000 against 3000-7000 for the other two. Those numbers cannot share one basis, so confirm the temperature in the current TDS before comparing quotes. Second, the page publishes no CAS, density, flash point or Tg; CAS 28768-32-3 comes from third-party databases and should be verified on the COA before customs or compliance work. Third, color stops at Gardner 10 or below and the liquid is yellow, so clear or decorative parts are not a fit.

The page also lists "fast curing speed at room temperature" while describing long pot life at process temperatures. Those statements pull against each other, as they do across multifunctional aniline systems; in practice the cure schedule depends on the curative and accelerator package, not on the resin alone. If a room-temperature schedule without postcure is a hard requirement, this is not the right resin family.

7.2 Incoming Inspection, Packaging, Storage and Safety

A four-line incoming check catches most lot problems: EEW by titration according to ASTM D1652 or ISO 3001, viscosity by the method stated in the TDS, color according to ASTM D1544, and volatiles on a fresh sample in duplicate. Storage follows the page: a well-ventilated area away from flames and sunlight, cap closed immediately after use, at least 12 months in the original packing at ambient temperature. Part-used drums deserve a nitrogen blanket; the epoxy groups are moisture-sensitive over long standing. All safety information is provided in the Material Safety Data Sheet, the governing document for handling and transport; check it before shipping, since the flash point is unpublished.

8. Frequently Asked Questions

What is the difference between YLSE-721, 721C and 721L?

One chemistry, three positionings. YLSE-721 carries the tightest EEW window at 105-120 g/eq and the high-purity label, YLSE-721C is priced for volume at EEW 110-125 g/eq, and YLSE-721L is the lower-viscosity version at 6000-11000 cps (25 °C) and EEW 110-125 g/eq. Verify the viscosity basis with the supplier first, per 7.1.

Which curing agents suit tetrafunctional epoxy resin YLSE-721?

Equivalent-weight arithmetic makes any polyfunctional amine or anhydride usable; Table 4 works the numbers for PACM, MHHPA, YLH-9101 and YLH-3002. For maximum service temperature, anhydride or aromatic amine systems with a staged postcure are standard; aliphatic amines cure faster but cap heat performance.

Why does the viscosity table show two temperature bases?

The column header reads 50 °C, but the YLSE-721L cell is annotated 25 °C. Epoxy viscosity falls steeply with temperature, so the two bases differ by a factor of several. Confirm the basis per grade; never quote a mixed comparison to a customer.

Can YLSE-721 replace a bisphenol A resin such as YLE-128?

No, and the substitution fails in both directions. YLE-128 flows at 11000-15000 mPa·s with EEW 184-190 g/eq and cures into a network that softens far below what YLSE-721 delivers; conversely, YLSE-721 costs more, processes stiffer, and its aniline network is wasted on ambient service parts. Choose by service temperature, not by habit.

What dosage should a first MHHPA trial with YLSE-721 use?

The Table 4 value is 136.1 phr at EEW 105 g/eq and 119.1 phr at EEW 120 g/eq, calculated with the 0.85 anhydride factor. Start near 120-135 phr with the usual 0.5-2 phr tertiary amine accelerator, run a gel time check, then adjust against DSC data.

How should YLSE-721 be stored after a drum is opened?

Follow the page: close the cap tightly after use, keep the drum in a ventilated area away from flames and sunlight, and use the contents within 12 months of manufacture. For a drum standing open for weeks, blanket it with dry nitrogen to limit moisture uptake and viscosity drift.

9. Conclusions

Tetrafunctional epoxy resin YLSE-721 gives formulators a documented route to high-crosslink, heat-resistant networks. Three grades cover EEW 105-125 g/eq, the calculated theoretical equivalent of 105.6 g/eq matches that window, and the published application fields are filament-wound composites and 200-260 °C structural adhesive. The open items are equally concrete: the grade table's viscosity basis needs TDS confirmation, CAS and physical constants are unpublished, and cure schedules must be validated per curative lot. Grade choice reduces to a single question: which constraint binds first, flow, price or purity.

10. References

1. Yolatech product page: 4,4'-Methylenebis(N,N-diglycidylaniline) YLSE-721/721C/721L, https://www.yolatech.com/44-methylenebisnn-diglycidylaniline-ylse-721721c721l (accessed 2026-10-26).

2. Yolatech product page: N,N-diglycidyl-4-glycidyloxyaniline YLSE-0500/0510/0510L, https://www.yolatech.com/44-methylenebisnn-diglycidylaniline (accessed 2026-10-26).

3. Yolatech product page: YLD-1240, https://www.yolatech.com/curing-agent-ylh-102g4 (accessed 2026-10-26).

4. Yolatech Technical Data Sheet, Material Safety Data Sheet and Certificate of Analysis for YLSE-721, YLSE-721C and YLSE-721L (available on request).

5. ASTM D1652, test method for epoxy content of epoxy resins.

6. ISO 3001, determination of epoxy equivalent.

7. ASTM D1544, Gardner color of transparent liquids.

leave a message

leave a message
If you are interested in our products and want to know more details,please leave a message here,we will reply you as soon as we can.
submit

home

products

WhatsApp

Contact Us