Trifunctional Glycidylamine Epoxy Resin: YLSE-0500 Failure Modes
Nov 13, 2026
Trifunctional glycidylamine epoxy resin YLSE-0500 is a low-viscosity triglycidyl p-aminophenol liquid at EEW 95-105 g/eq, CAS 5026-74-4. Two siblings, YLSE-0510 and YLSE-0510L, reach 400-1,000 cps at 25 °C. Flow fills fine windings and thin sections, and that same reactivity can char a 5 kg casting.
Figure 1. YLSE-0510 in the beaker and a cured disc from the same lot. Colour and thin flow are what buyers check first; neither predicts a 5 kg mould.
1. Introduction
All three grades share one molecule: N,N-diglycidyl-4-glycidyloxyaniline, a triglycidyl ether of p-aminophenol with two glycidyl groups on the nitrogen and one on the phenolic oxygen. A bisphenol A liquid carries 2.0.
Low viscosity is why buyers pick this family: YLSE-0510 pours at 400-900 cps, so it wets glass roving and copper inserts without solvent. The cost appears after demoulding, when castings crack at inserts and cores char.
2. Materials and Methods: Specification Basis for Trifunctional Glycidylamine Epoxy Resin
2.1 Product identification and published specification
One chemistry at three viscosity bands, so one identity table covers all three.
Table 1. Identity data for YLSE-0500, YLSE-0510 and YLSE-0510L as published, accessed 2026-11-13.
Item
YLSE-0500 / 0510 / 0510L
Chemical name
N,N-diglycidyl-4-glycidyloxyaniline
CAS number
5026-74-4
Epoxide groups
3 (trifunctional)
Molecular formula
C15H19NO4 (calculated, 277.32 g/mol)
Package
Drum
Shelf life
At least 12 months, original closed drum, ambient
Table 2 repeats the parameter block as printed; a dash means empty.
Table 2. Published parameters for YLSE-0500, YLSE-0510 and YLSE-0510L, accessed 2026-11-13.
Property
YLSE-0500
YLSE-0510
YLSE-0510L
Appearance
Brown liquid
Yellow liquid
Yellow liquid
EEW, g/eq
95-105
93-106
95-105
Viscosity, cps at 25 °C
1,500-6,000
400-900
500-1,000
Volatiles, %
Max. 1.5
Max. 1.0
Max. 1.0
Total chlorine, ppm
-
-
Max. 800
Hydrolyzable chlorine, ppm
2,000
1,000
Max. 200
Epoxy equivalent weight is titrated under ASTM D1652, and each lot carries that value on its certificate. Viscosity is quoted at 25 °C, where a 10 °C fall can double the figure.
2.2 Test methods and data sources
Two sources feed this report: the published pages and arithmetic. EEW windows, viscosities and chlorine limits are quoted as printed; molecular weight and hardener weights are calculated and labelled as such.
The theoretical EEW of 92.4 g/eq is 277.32 g/mol divided by three epoxide groups. Published windows sit above it because lots carry a few percent of higher oligomers. Duplicate titration is normal; treat one reading as provisional.
3. Results and Discussion: Failure Modes of Trifunctional Glycidylamine Epoxy Resin
3.1 Structure, enthalpy and what follows
Three epoxide groups in 277 g/mol give about 10.5 eq/kg, against 5.3 eq/kg at EEW 188. Double the sites, double the heat.
Ring opening of a glycidyl ether by an amine releases about 105 kJ/mol, so a kilogram of YLSE-0500 carries near 1,050 kJ. At 1.7 kJ/kg·K, an adiabatic core would pass 500 °C.
Geometry decides. A 100 g cup in a 25 °C room sheds heat through the wall. A 5 kg block in a steel mould keeps it, so charring starts at the core.
The aniline nitrogen also accelerates the reaction, so the resin gels sooner than 400 cps suggests. Gel time shortens as the shop warms, and not linearly.
Table 3. Field symptoms, causes and countermeasures for YLSE-0500, YLSE-0510 and YLSE-0510L castings.
Symptom
Cause
Countermeasure
Smoke, dark core
Exotherm above 2 kg with a fast aliphatic amine
Cap batch mass, chill the mould, or use an anhydride
Cracks at inserts
Shrinkage stress locked in by fast gel
Stage the cure, pre-warm inserts to 60 °C
Tg below 200 °C
Hardener dosed from the datasheet midpoint
Recalculate phr, post-cure 2 h at 160 °C
Bubbles, pinholes
1.5% volatiles plus air held by a 400 cps liquid
Degas 10-15 min at 5 mbar
Leakage current rise
2,000 ppm hydrolyzable chlorine in a DC field
Move the part to YLSE-0510L at 200 ppm
Brown resin rejected
The 0500 grade is brown by specification
Judge against the grade descriptor
Gel in the line
Pot life collapsed at 35 °C ambient
Hold at 25-30 °C, meter on demand
Two rows of Table 3 are grade-selection problems, not process problems. Chlorine and colour cannot be degassed, filtered or post-cured out of a part.
3.2 Comparison with alternative systems
The closest alternative is YLSE-0600, the 3-isomer of the same molecule, at 10,000-25,000 cps: same formula, fifty times the viscosity.
Table 4. Property comparison, with EEW-derived heats for ranking only: YLSE-0500 family against YLSE-0600, YLSE-721 and a bisphenol A liquid.
Property
YLSE-0500 family
YLSE-0600
YLSE-721
YLE-128
Epoxide groups
3
3
4
2
EEW, g/eq
93-106
100-110
105-125
184-190
Viscosity at 25 °C, cps
400-6,000
10,000-25,000
3,000-7,000
11,000-15,000
Hydrolyzable chlorine, ppm
200-2,000
Not published
Not published
Max. 500
Heat per kg at full cure
About 1,050 kJ
About 980 kJ
About 830 kJ
About 540 kJ
Typical role
Casting, RTM, winding
Adhesive, laminating
Aerospace composites
General purpose
Pick YLSE-0600 when the resin must stay put, and 0500 or 0510 when it must flow into a closed mould. Their EEW windows overlap, so viscosity settles it.
4. Formulation and Dosage Calculation
Hardener weight follows one line: phr = 100 × AHEW ÷ EEW. Stoichiometry failures start with dosing from the EEW midpoint instead of the lot certificate.
Table 5. Hardener demand per 100 g of resin at three EEW points inside the published window.
Hardener
AHEW, g/eq
phr at EEW 95
phr at EEW 100
phr at EEW 106
Diethylenetriamine, theoretical
20.6
21.7
20.6
19.4
YLH-6005 polyetheramine
95
100.0
95.0
89.6
MHHPA anhydride, k = 0.85
142.96
150.5
143.0
134.9
Worked example. A 20 kg batch of YLSE-0500 arrives at 104 g/eq. Against YLH-6005 at AHEW 95 the correct addition is 91.3 phr, or 18.26 kg. The nominal 100 g/eq gives 95.0 phr, or 19.0 kg, so the gap is 0.74 kg and 4% excess amine.
Surplus amine plasticises the network, lowers Tg and raises water uptake. A 4% surplus can pull a 200 °C system into the 180s, and the drop gets blamed on the resin.
Anhydrides invert the arithmetic. MHHPA carries 168.19 g/eq, and practice applies 0.85 of that, giving 143 phr at EEW 100. The heavy addition is why anhydride casting runs at 80-100 °C.
5. Processing Notes and Operating Window
Four settings keep it workable: batch mass, resin temperature, vacuum, and cure ramp.
• Cap batches at 2 kg with an aliphatic amine at 25 °C, and halve that above 30 °C.
• Hold resin at 25-30 °C. Warming to 40 °C halves pot life unless the section is under 3 mm.
• Degas at 5 mbar for 10-15 minutes. The 1.5% volatile limit on YLSE-0500 makes the step non-optional.
• If the system is aromatic-amine and aimed at the 200 °C class, ramp to 80 °C, hold 2 h, then post-cure 2 h at 160 °C.
Figure 2. Degassing a YLSE-0510 mix at 5 mbar. Foam rises, collapses, then the resin clears from the centre outwards.
Bubbles that survive degassing usually come from the hardener. Polyetheramine takes up water in an open drum, and 0.5% water there foams a casting that looked clear in the cup.
6. Applications
The published list runs from electrical casting to composite winding; grade choice follows chlorine and viscosity.
Table 6. Grade selection by application and process.
Application
Process
Grade
Reason
HV bushings, insulators
APG, vacuum casting
YLSE-0510L
200 ppm hydrolyzable chlorine
Micro-motor sealing
Vacuum casting
YLSE-0510
400-900 cps wets fine wire
Carbon fibre winding
Filament winding
YLSE-0510
Low drag through the bath
RTM and VARTM panels
Resin injection
YLSE-0510
Fills a 2 m flow path at 25 °C
High-temperature adhesive
Hand mix, bonded joint
YLSE-0500
1,500-6,000 cps stays on the bondline
Reactive diluent
Blend at 5-15 phr
YLSE-0510L
Trifunctional, so Tg retention beats BGE
Figure 3. A cast insulator plate with brass inserts, moulded from YLSE-0510L. Shrinkage stress concentrates at the bosses, where the cure ramp matters more than the mix ratio.
For high-voltage parts the 200 ppm figure matters more than viscosity. Ionic chlorine migrates under a DC field in humid air, so leakage current appears months after the part passed its test.
7. Limitations and Material Verification
7.1 Known limitations and unsuitable cases
The 200 °C glass transition figure is a class statement for post-cured systems, not a measured value. The product URL still reads 44-methylenebisnn-diglycidylaniline while the page describes the triglycidyl p-aminophenol grades, so order by CAS. Grade windows differ inside one family, 93-106 g/eq across the three, so the lot certificate decides.
Chlorine is the other constraint. At 2,000 ppm, hydrolyzable chlorine rules YLSE-0500 out of high-voltage insulation, while YLSE-0510L caps that at 200. The pages print no Gardner number; appearance is brown for YLSE-0500 and yellow for the other two, so a dark drum is specification, not age.
Do not run unfilled sections above 5 kg with an aliphatic amine, or specify YLSE-0510 where the drawing names a chlorine ceiling under 200 ppm.
7.2 Incoming verification, packaging and storage
Checks for every drum: EEW by titration with n = 3, viscosity at 25 °C, and water by Karl Fischer according to ASTM E203. Chlorine matters only for electrical parts, and then on every lot.
Viscosity is measured at 25 °C under ASTM D445, and colour, where quoted, under ASTM D1544. If a drum titrates at 104 g/eq it still sits inside the YLSE-0510 window, and the dosage follows the titration.
Storage runs 12 months from manufacture in the closed original drum. Resin from a warm warehouse still titrates in window, and still gels faster.
Safety data comes from the MSDS, limits from the TDS. Skin contact is the routine risk with glycidyl ethers, and gloves rated for epoxy beat nitrile examination gloves.
8. Frequently Asked Questions
What separates YLSE-0500, YLSE-0510 and YLSE-0510L?
Viscosity and chlorine. YLSE-0500 pours at 1,500-6,000 cps with 2,000 ppm hydrolyzable chlorine, YLSE-0510 at 400-900 cps with 1,000 ppm, YLSE-0510L at 500-1,000 cps with 200 ppm.
Why did my casting crack the day after demoulding?
Fast gel at high crosslink density locks shrinkage stress into the part, and it concentrates at inserts. Stage the cure, pre-warm inserts, and hold the part at 60 °C before the post-cure ramp.
Can YLSE-0500 be cured at room temperature with DETA?
In thin sections, yes. Above about 2 kg the exotherm outruns the mould, and the core chars while the surface still looks sound. Chill the mould or move to an anhydride above that mass.
Why is the measured Tg below the 200 °C class figure?
Check two things first: whether the hardener weight came from the lot EEW, and whether the post-cure reached 160 °C in the core. Both give the same 20-40 °C shortfall.
Is YLSE-0510L suitable for high-voltage insulation?
It is the grade intended for that duty, at 200 ppm hydrolyzable chlorine. Suitability still depends on the cured system, the design field and the applicable standard; a low chlorine figure is not a certification.
Can these grades work as reactive diluents?
Yes, at 5-15 phr in a bisphenol A or phenolic system. Trifunctional dilution costs less Tg than butyl ether and more per kilogram, so the trade-off is thickness against budget.
9. Conclusions
YLSE-0500, YLSE-0510 and YLSE-0510L are one triglycidyl p-aminophenol molecule at three viscosity and purity bands, and the band decides the application.
Cure enthalpy near 1,050 kJ/kg sits behind most field failures here. Mass limits, a staged cure and lot-specific hardener weights address it; extra degassing does not.
Chlorine rather than viscosity separates 0510L from 0510, and 200 ppm against 2,000 ppm is a factor of ten. Take EEW from the certificate: on a 20 kg batch the midpoint habit costs 0.74 kg of hardener.
10. References
1. Yolatech, N,N-diglycidyl-4-glycidyloxyaniline YLSE-0500 / 0510 / 0510L, https://www.yolatech.com/44-methylenebisnn-diglycidylaniline (accessed 2026-11-13).
2. Yolatech, 3-glycidyloxy-N,N-diglycidylaniline YLSE-0600, https://www.yolatech.com/3-glycidyloxy-nn-diglycidylaniline-ylse-0600-afg-90m-cas-71604-74-5 (accessed 2026-11-13).
3. Yolatech, 4,4'-methylenebis(N,N-diglycidylaniline) YLSE-721, https://www.yolatech.com/44-methylenebisnn-diglycidylaniline-ylse-721721c721l (accessed 2026-11-13).
4. Yolatech Technical Data Sheet (TDS) and Certificate of Analysis (COA) for YLSE-0500, YLSE-0510 and YLSE-0510L, CAS 5026-74-4.
5. ASTM D1652, epoxy content of epoxy resins; ISO 3001, epoxide equivalent.
6. ASTM E203, water by Karl Fischer titration; ASTM D445, kinematic viscosity; ASTM D1544, Gardner colour.
7. Yolatech, bisphenol A epoxy resin grade table, https://www.yolatech.com/bisphenol-a-epoxy-resin (accessed 2026-11-13).
Read More